C60R is a non-alloy steel with many excellent properties and a wide range of applications. It is a type of carbon spring steel with excellent metallurgical quality (high coating degree and uniformity) and good surface quality (strict control of surface defects and demoulding). After heat treatment or cold drawing heat treatment, C60R obtains extremely high strength, hardness, elasticity and appropriate toughness and plasticity. With the same surface condition and complete hardening, C60R is also suitable for tool manufacturing, showing its applicability in tool and mold manufacturing. This strength and range of applications make it one of the most important materials in industry.
Availability:
Quantity:
facebook sharing button
twitter sharing button
line sharing button
wechat sharing button
linkedin sharing button
pinterest sharing button
whatsapp sharing button
sharethis sharing button

CHEMICAL COMPOSITION

C: 0.57-0.65

Si: ≤0.40

Mn: 0.60-0.90

P: ≤0.035

S: 0.020-0.040

Cr: ≤ 0.40

Ni: ≤ 0.40

Mo: ≤ 0.10

Cr+Ni+Mo: ≤ 0.63


MECHANICAL PROPERTIES

Young's modulus: 200000MPa

Tensile strength: 650-880MPa

Elongation: 8-25%

Fatigue: 275MPa

Yield strength: 350-550MPa



HEAT TREATMENT

Soft Annealing:Heat to 650-700oC, cool slowly in furnace. This will produce a maximum Brinell hardness of 241.


Normalizing:Normalizing temperature: 820-850oC.


Hardening:Harden from a temperature of 800-830oC, 810-840oC followed by water or oil quenching.


Tempering:Tempering temperature: 540-680oC.


The Management and Staff at Union Steel, have a firm belief that by identifying the customers’ needs, we can achieve the best results for all. Union Steel warmly welcomes friends around the world to cooperate with us.

Quick Links

Contact Us

Tel: +86-24-81267300
Phone: +86-18904079192
Add: No. 237, Shenbei West Road, Yuhong District, Shenyang City, Liaoning Province

Product Category

Keep In Touch
Contact
Copyright ©  2024 Union Steel. All rights reserved.  SitemapPrivacy Policy  辽ICP备2024037155号-1