CHEMICAL COMPOSITION
C: 0.37-0.42
Si: 0.90~1.20
Mn: 0.30~0.50
P: ≤0.030
S: ≤0.030
Cr: 4.80~5.50
Mo: 1.20~1.50
V: 0.90~1.10
MECHANICAL PROPERTIES
Hardness: 48-52 HRC (Rockwell hardness)
Tensile strength: 1550-1850 MPa (MPa)
Yield strength: Its yield strength is usually 1400-1600 MPa
PHYSICAL PROPERTIES
Density: 7.31 g/cm³
Modulus of elasticity:
At 20°C, 212000 MPa
Shear modulus: 825000 MPa
Poisson's ratio: 0.288
Thermal conductivity: The thermal conductivity of 1.2344 changes at different temperatures, for example,
At 20°C, it is 36.0 W/(m·K)
At 100°C, it is 33.4 W/(m·K), and so on.
HEAT TREATMENT
Isothermal annealing: annealing temperature (850±10)°C, holding for 2 hours, cooling to (720±10)°C in the furnace, holding for 4 hours, cooling the furnace to below 500°C, air cooling after exiting the furnace, hardness ≤229HBW.
High temperature tempering: Tempering temperature (730 ±10)°C, heat preservation for 2 hours, furnace cooling to ≤500°C, air cooling after exiting the furnace.
Quenching and tempering: quenching temperature 850-880°C, oil cooling, hardness 50-52HRC; tempering temperature 580-640°C, air cooling out of the furnace, hardness 28-36HRC.
Pre-hardening treatment: heating temperature 860-900°C, oil cooling, tempering temperature 570-700°C, air cooling, tempering hardness 28-35HRC.
FORGING
Forging temperature range is 1050-850℃